旋流器与细筛联合分级工艺在某铁矿的应用
山东某铁矿二次分级旋流器应用效果研究

山东某铁矿二次分级旋流器应用效果研究摘要:本文针对山东某铁矿在设计投产阶段遇到产量不达标,铁精粉品位低,磨矿耗能大等问题,研究后发现旋流器的工况不稳定是问题的关键。
经过对旋流器给料、底流、溢流产品的粒度、品位分析,发现旋流器分选作业中出现的分级效率低,铁矿物反富集等不正常现,导致上下游相关设备达不到正常生产的要求。
针对现场生产情况提出相关解决方案,最终选厂问题得到解决,生产情况趋向稳定,达到设计指标。
关键词:旋流器粒度品位分级效率Abstract: this paper put into production in shandong some iron ore design phase output is not meet the standard, iron essence pink low grade, grinding energy consumption, research found that the operation condition of the hydrocyclone is instability is the key to the problem. “After the v ortex is feeding, bottom flow, overflow product size, grade analysis, found the hydrocyclone separation assignments appear the grading efficiency is low, the content such as iron ore enrichment is not normal, lead to upstream and downstream related equipment can not reach the normal production requirements. According to the field production related solutions are put forward, finally the mill problems can be solved, the production situation trend stability and achieved the design index.Keywords: rotary flow particle size grade the classification efficiency中图分类号:P57文献标识码:A 文章编号:1概述随着资源的不断消耗,近年来入选矿石“贫、细、杂”的特点越来越突出。
河北某铁矿选矿分级设备对比与实践

1 分 级 设 备 原 理 及 特 点 分 析
1 . 1 螺 旋分 级机
2 分 级 效 果 对 比实 践 分 析
2 . 1 生产 工艺 指标对 比分 析
螺旋分选机是将细磨后的矿浆从位于沉降区中 部 的给料 口给入水 槽 , 螺 旋低 速转 动 , 轻 细颗 粒流 到 溢流堰 处溢 出 , 粗 中颗 粒则沉 降 到槽 底 , 由螺 旋输 送 到排料 口返 回磨机 再磨 。 1 . 2 水 力旋 流器 旋 流器 是将 给入 矿物料 沿切线 从 圆筒 内壁高 速 给人 , 在离 心力 、 介 质 黏滞 阻力 、 浮力 、 重力 等力 场 的 作用 下 , 粗 颗粒 、 大 密度 的颗 粒 向 周边 运 动 , 通 过 锥 形体从沉砂 口排出; 细颗粒 、 低密度的颗粒向中心运
结构简单 , 设备投资少 , 运行成本低 , 安装与操作简 便, 体积小 , 分级效率高 , 处理能力大且 占用空间小 。 直线振 动筛 能够 强制分 级 , 分 级效 率 一 般可 提 高 1 5 2 0个 百 分 点 , 可 有 效 防止 1次 磨 机 对 矿 石 的 过 磨, 但 粒度 调整 不方便 。
宁小永 ( 1 9 8 0 一) , 男, 工程师 , 0 6 4 4 0 4河北省迁安市滨河村 。
河北 某铁矿 目前 有 1 3个磨 选 系列 , 磨 选工 艺 流
程中的 1 次磨矿分级作业 中分级设备为旋 流器 、 高 堰 双螺旋 分 级 机 ( 以下 简 称 分 级 机 ) 和 直 线 筛 3种 设备 。其 中, 1 系列分级设备使用 4 , 6 6 0 m m旋流器 组, 2系列分级设备使用螺旋分级机 ; 1 、 2系列原矿 性质、 磨机型号以及选别工艺及设备配置等其他工 作 条件 一 样 ; 3~1 1系列 生 产 的铁 精 矿 产 品粒 度 在 0 . 0 7 4 m m 7 0 %左右 , 除分 级 设 备 不 同 以外 , 原 矿 性质、 磨机型号以及选别工艺及设备配置等其他工 作 条件 一 样 ; 3—5系列 分 级 设 备 使 用 2 F L G 一 2 0 0 0 mm×8 2 0 0 mm型螺 旋分 级机 , 8~1 1系列分 级设 备
旋流器在某矿充填工艺中的应用

起来 , 形成不 了均匀 的浆体 , 沉在 了砂仓底部 ; ④相 关 突 出问题 所带来 的一 系列成 本 问题 。
3 系统 改造
为 提高 尾 砂 利 用 率 , 对原 充填系统进 行改 造。 具体 改造 方 式 是 在 一 个 系 列 的尾 砂 仓 顶 加 装 旋 流 器, 进 砂 先通 过 仓顶 旋 流 器 直 接 流 入 仓底 。改 造 后
1 . 2 充填站 建设 最 初建 设 有 2套 充 填 系统 , 与 国 内大 多数 矿 山
的充填工艺基本相同, 每套 系统建设有 2个尾砂仓 和1 个 水 泥仓 , 立 式 砂 仓 直径 为 1 0 m, 水 泥 仓 直 径
为5 m, 砂仓 有效 容积 为 1 5 0 0 m , 砂仓 底 部平 台为
计量 , 下 方平 台为双 轴搅拌 机 , 用于对 砂浆 的初 步搅 拌, 双轴 搅拌 机下方 为高 速活化 搅拌 机 , 用 于砂 浆及 水 泥 的活化搅 拌 , 直接 通 过 井下 充 填 管 道进 入 充 填 采场 , 充填站 系统见 图 1 。
的前提下如何提高尾砂利用率仍是一项关键难题。 某 矿 目前 采 用 全尾 砂 胶结 充 填采 矿 法 , 年 充填
尾砂 的利 用率 很低 , 因 中间省去 了浓缩 池 , 尾砂 直接 打 入 充填 砂 仓 , 尽 管砂 仓 直 径 为 1 0 m, 但 选 厂尾 砂 粒 径很 小 , 一 大部 分 细颗 粒 尾 砂 和极 细 尾 砂 几乎 没 来 得及 沉底便 溢 流 出去 , 排 至临 时尾矿 库 , 经 过一 段
空区量 要在 9 0 % 左右 方可 保证 采 充 平衡 , 但 尾 砂利
旋流器分级反富集累积对某铁矿选矿指标影响试验

图 1 选矿工艺流程 表 1 一段旋流器溢流与沉砂筛析结果
粒级 /mm
一段旋流器溢流 产率 /% 铁品位 /%
+6
ቤተ መጻሕፍቲ ባይዱ
3~6
2~3
0.83~2
0.27~0.83 3.57
16.03
0.15~0.27 10.33 21.23
0.106~0.15 7.14
28.89
0.074~0.106 6.18
31.04
在生产现场对选矿工艺流程一段旋流器溢流 (一段溢流)和沉砂、二段旋流器溢流(二段溢流)、 三段旋流器溢流(三段溢流)进行取样,开展筛析对 比与弱磁选试验。 2.1 一段旋流器分级产品筛析试验
对一段旋流器溢流与沉砂进行筛析试验,结果 见表 1。
朱立杰(1986—),男,工程师,063700河北省唐山市滦县。
表 3 二段旋流器溢流一段弱磁选试验结果 %
产品 一段弱磁精矿
尾矿 给矿
产率 39.19 60.81 100.00
铁品位 60.67 14.33 32.49
细度(-0.074mm) 79.0
表 4 三段旋流器溢流一段弱磁选试验结果 %
产品 一段弱磁精矿
尾矿 给矿
产率 27.55 72.45 100.00
铁品位 60.84 11.92 25.40
细度(-0.074mm) 98.0
由表 2~表 4可知,一段溢流、二段溢流、三段 溢流一段 弱 磁 精 矿 细 度 -0074mm 含 量 分 别 为 630%、790%、980%,铁 品 位 分 别 为 5827%、 6067%、6084%,尽管 细 度 增 加 明 显,但 一 段 弱 磁 精矿铁品位变化不大。相比一段溢流,二段溢流一 段弱磁精矿细度 -0074mm含量增加了 16个百分 点,但铁品位只提高了 240个百分点;相比二段溢 流,三段溢流一段弱磁精矿细度 -0074mm含量增 加了 19个百分点,但铁品位只提高了 017个百分 点,说明旋流器连续分级造成的反富集累积对选别 效果影响较大。为进一步分析旋流器连续分级反富 集累积的影响,分别对各段旋流器溢流一段弱磁精 矿开展磨矿—弱磁选试验分析。 2.3 旋流器溢流二段弱磁选试验 2.3.1 一段溢流二段弱磁选试验
旋流器与高频细筛组合作业在白象山选矿厂的应用

稳 定 。选厂 通过 控制 旋流 器给矿 浓度 与给矿 压 力参数 、 调 整 高频 细 筛筛孔尺 寸 , 提 高 了给入 淘洗机 矿料 细粒级 的含 量 , 大幅提 升 了磨 选 系统的 生产 效率 , 选厂 增效 显 著 。
关键 词 水 力旋 流 器 分级 效 率 高频 细 筛 组 合分 级
对 高 频 细筛 进 行 改 造前 多 粒 级 分 析 , 分析 结 果
见表 2 。
县 太 白镇 。
由表2 可知 , 高频 细筛筛下物 一 0 . 0 7 4 m m 粒级
1 3
总第 5 8 3期
表1 调 整 前 旋 流 器 参 数指 标
现 代矿 业
%
2 0 1 7年 1 1月第 1 1期
S e r i a l N o . 5 8 3 No v e mb e r . 2 0 1 7
现
代
矿
业
M0D ERN MI NI NG
总 第5 8 3期 2 0 1 7 年1 1月 第 1 1 期
旋 流器 与高 频 细 筛 组 合 作 业在 白象 山选 矿厂 的应 用
王 金 行 陆 虎 杨 松 付
1 选厂概 况
1 . 1 白象 山矿矿 石性 质
白象山铁矿床为气化高温热液交代矿床 , 矿床
中主要 的金 属 矿 物 为 磁 铁 矿 , 含量为 4 6 . 3 %, 主 要 脉 石矿 物为 白云石 、 方 解 石 等 碳 酸 盐类 矿物 。磁 铁 矿呈 各种 不规 则粒 状 , 粒度 微细 , 主要 分 布于 一0 . 0 5 m m 粒级 , 分布率为 7 9 4 9 %, 其 中 一1 0 m 粒 级 占 2 9 . 1 6 %, 因此 矿石 中主 要 有 用 铁 矿 物属 细 粒 嵌 布 。 正是 由于 磁 铁 矿 的 细 粒 分 布 , 为 达 到 设 计 铁 品 位 6 3 . 5 % 的指标 , 生 产 中必 须严 格控 制磨 矿粒 度 。 1 . 2 磨 选工 艺流 程 人磨 物料 来 自湿抛 工序 精矿 , 一 段 MQ Y 3 6 6 0溢 流 型球磨 机 与 1段 F X . 6 6 0 一 G X旋 流 器 组成 闭路 , 合 格粒 级 (一0 . 0 7 4 m m 6 0 %) 物料经 1 段 粗 选 进 入 二 段F X . 3 5 0 . G X旋流器组分级 , 与 MQ Y 4 6 7 5溢 流 型 球磨 机 形 成 闭路 磨 矿 , 2段 磨 矿 后 最 终 设计 粒 度 为
海王精细分级旋流器在某特大型铁矿细粒磨矿分级工艺中的应用

图5 渐 开 线 旋 流 器 进 料 体 速 度 分布
方式 、 锥体结构及柱段高度等, 达到提高旋流器分级 精 度 及分 级效 率 的 目的 , 从 而 在 保 证 溢 流 细度 的前 提下 降低 沉砂 夹细 及返 砂 比 。 ( 1 ) 优化旋 流 器 的进 料 方式 和 锥 体 结 构 。旋 流 器 的进料方 式和 锥体 结 构是 影 响旋 流器 分级 效 率 的 主要因素 , 威海市海王旋流器有限公司研发的精细分 级 0 o I T l l n 旋流器采用了改进型的螺旋线进料体和 复合锥体结构 ( 见图2 ) 。螺旋线入料方式是一种进 料阻力小 、 紊流 程度 小 的先进 结 构 。流 场 研究 表 明, 颗粒在进 料管腔 中旋转 过程 中进料 管 内侧 和外 侧 同
1 7 5
路9 5号 。
总第 5 8 3期
现代 矿 业
2 0 1 7年 1 1月 第 1 1 期
时出现密度增 大现象 ( 见图 3 ) , 说 明颗粒在 进料 管 中
进 行排列 和分离 , 粗颗 粒 更靠 近外 侧 、 细颗 粒 更 靠 近 内侧 , 从而提高 了分级 精度 及分 级 效率 ; 另 一 方 面螺 旋进 料体 的进 料紊 流小 , 通过 C F D模 拟 螺 旋线 进 料
王 磊 郑纪 民 齐加 刚 王德 明
( 威 海 市海王 旋流 器有 限公 司)
摘
要
针 对 常规旋 流 器存在 的 分级 效率低 、 循 环 负荷过 高等 问题 , 威 海 市海王 旋流 器有 限公
水力旋流器在铁矿选矿中的应用及发展

设计与研究本文引用格式:张鹏飞,谢海云,陈禄政,等.水力旋流器在铁矿选矿中的应用及发展[J]. 新型工业化,2016,6(4):8-15.DOI:10.19335/ki.2095-6649.2016.04.002水力旋流器在铁矿选矿中的应用及发展张鹏飞1,2,谢海云1,2,陈禄政1,李圆洪1,丁超1,童雄1(1.昆明理工大学国土资源工程学院,云南昆明 650093;2.省部共建复杂有色金属资源清洁利用国家重点实验室,云南 昆明 650093)摘要:我国铁矿资源较丰富但品质普遍不高,需要进行高效选矿富集。
水力旋流器在铁矿选矿中的应用日益广泛。
本文在对我国铁矿石资源特征及分选概况总结的基础上,分析了水力旋流器的分选过程、流场特征及分级过程的粒度特征等;阐述了水力旋流器在铁矿选矿中的分级、脱水等方面的应用情况,并指出了应用中存在的问题,对水力旋流器在铁矿选矿中的发展趋势进行了分析。
论文对提高铁矿资源的选矿利用具有重要的指导意义。
关键词:水力旋流器;铁矿;选矿;分级Application and Development of Hydrocyclone in Iron Ore BeneficiationZHANG Peng-fei1, 2, XIE Hai-yun1, 2, CHEN Lu-zheng1, LI Yuan-hong1, DING Chao1, TONG Xiong1(1.Faculty of Land Resource Engineering, Kunming University of Science and Technology, Kunming 650093, China; 2. State Key Laboratory of Complex Nonferrous Metal Resource Clean Utilization, Kunming 650093, China)Abstract: There are a lot of iron ore resources in China, but the quality of ore is generally poor. It needs to be concentrated efficiently by mineral processing methods. Hydrocyclone has been used increasingly in iron ore beneficiation. Based on the char-acteristics of iron ore in China and its separation, It analyzes the hydrocyclone separation process, the flow field characteristics and the grain size characteristics of classification process, This paper expounds the application of the hydrocyclone classificationin iron ore beneficiation and dehydration etc, points out the problems existing in the application, and analyzes the development trend of hydrocyclone in iron ore beneficiation .This paper has an important guiding significance in improving the concentrationof iron ore.Keywords: Hydrocyclone; Iron ore; Beneficiation; Classification我国铁矿资源总量丰富,截止2007年底,全国铁矿石资源储量680亿吨。
旋流器串联分级在磁铁矿选矿中的应用研究

第3 2卷 第 4期
20 0 8年 8月
中
国
钼
业
V 13 o 4 o. 2 N .
Aug t 2 8 us 00
C NA M0L HI YBDENUM NDUS I TRY
旋 流 器 串联 分 级 在 磁铁 矿选 矿 中的应 用 研 究
王鹏程 徐 引行 谢建宏 李宏伟 ห้องสมุดไป่ตู้ , ,
(. 1西安建筑科技大学材料学 院, 陕西 西安 7 05 ) 10 5
(. 2 金堆城钼业汝阳有限责任公 司 , 河南 汝 阳 4 10 ) 7 20 摘 要: 为了解决 细粒级磨矿 的分级 问题 , 在磨矿分级 回路 中 , 以串联旋 流器组作 为分级设 备 , 高 了磨 矿浓度和 提
铁矿 、 赤铁 矿 、 铜 矿 、 黄 方铅 矿 、 闪锌 矿 , 石 矿 物 主 脉
1 铁 精 矿 品位 低 的 原 因分 析
选铁 车 间的原 矿是选 钼 车间钼 扫选 的尾矿 。钼 粗扫 选 的 目的是扔 掉 大 量 的非 钼 矿 物 和 脉石 矿 物 , 且要 保证 一定 的 钼 回收 率 , 因此 , 磨粒 度不 很 细 , 初 生产 中 一 .7 m仅 占 7 % 左右 。在 选 铁 车间粗 004m 0 选 且再 磨 以后 , 0 0 3mm也 只有 5 . % 。 一 .4 45
Ab ta t I r e o s le t e f e— g i d n r d ain p o l m ,t e s ra y ln s tk n a h r d ain sr c : n o d r t o v h n i rn i g g a u t r b e o h e lcco e i a e s te ga u t i o e u p n i u ai n o r d n q i me ti cr lt f i i g—g a u t g t e e gi d n e st n f c e c r n a c d g e t ,te n c o g n r d ai , h n t rn i g d n i a d e iin y a ee h n e r al h n h y y s e fa t n o 一0 0 3 i r ci f z o . 4 mm o g ei s a h e e f r ma n t e i c iv d.a d a h g u l y i n c n e tae p o u t n i o t ie t n ih q a i r o c n r t r d ci s b an d t o o
- 1、下载文档前请自行甄别文档内容的完整性,平台不提供额外的编辑、内容补充、找答案等附加服务。
- 2、"仅部分预览"的文档,不可在线预览部分如存在完整性等问题,可反馈申请退款(可完整预览的文档不适用该条件!)。
- 3、如文档侵犯您的权益,请联系客服反馈,我们会尽快为您处理(人工客服工作时间:9:00-18:30)。
11 2
铁精 矿
尾 矿
图 1 原 工 艺 流 程
22 原 工 艺流 程存在 的主要 问题 . 原流 程 中 由于 2段 细 筛 的筛 分 面 积小 , 筛分 效
张润身 席江伟等: 旋流器与细筛联合分级工艺在 某铁矿的应用 率偏低 , 仅为 1.% ~ 9 8 使得 大量 的细颗粒 04 3 . %, 造成 过磨 , 约 了 精 矿 品位 和 金 属 回 收 率 的提 高 。 制
() 1 由于 矿 石 结 晶粒 度 为 0 0 . 1—0 1 m, . 5 m 属
为分级设备 , 比细筛更适合于细粒级矿石分级 , 分级
效率 更高 。
于 不均 匀细 粒嵌 布 , 矿 细度需 要 一 .4 磨 0 08mm含 量
( ) 段磨 矿采用水力旋流器组 和细筛联合分 23 级工艺 , 降低了入筛物料浓度 , 提高了人筛物料 中合
表 5 细 筛 分 级 考 查 结 果 %
环带来的一系列问题 , 简化理顺 了流程 , 提高了分级 效率和磨矿效果 , 稳定 了精矿品位 , 降低 了工人劳动
强度 , 高 了综 合 效益 , 为其他 矿 山提供 了经验 借 提 并
鉴。
( 稿 日期 2 1 - -7 收 0 20 2 ) 4
流程 循环 负 荷 过 大 , 机 平 均 台 时 能 力 只 有 4 . 磨 27 t( ・ )单 位 磨 矿 分 级 电耗 高 达 2 .2k / , /台 h, 67 Wht 影 响 到 2 3段 磨 机 的磨 矿效 果 ; 、 磨 机 磨 矿 浓 、 2 3段
度 小 于 7 % , 排 矿 一0 0 4 m 细 度 差 不 超 过 0 给 .7 m 5 ; % 流程运 转 过 程 中跑 冒现 象 严 重 , 时制 约 了 1 同
表 2 磨 矿 效 果 考 查 结果 %
3 流程优化方案
3 1 工艺 优化 内容 .
经过 多次 考查论 证 , 确定 了工 艺 流程优 化方 案 。
用3 套水力旋流器组作 为 2段磨矿 的控 制分级设 备 , 代原 细筛 分 级 和 浓缩 磁选 机 。用 2套 水 力 水 替 力 旋 流器组 作 为 3段 磨矿 的控 制分 级 和入磨 前 的浓
选
晶结构 , 条纹状或条带状构造 。主要金属矿物为磁 铁矿 , 属于细粒不均匀嵌布 , 晶粒 度一般在 00 结 .1 0 1 m。脉石矿 物 主要 为 石英 和铁 闪 石 。矿 石 .5m
~
的氧化 程 度很低 , 为原 生矿 , 均 矿石 硬度 厂=1 2—1 。 4
对原矿进行铁物相分析 , 其结果见表 1 。
缩设 备 , 水力 旋 流器 组溢 流再 经过 细筛控 制 分级 , 实
表 3 细 筛 分 级 考查 结 果 %
现水 力 旋流 器组 和细 筛 的联合 分级 工艺 。将 水力 旋 流 器组 替代 下 来 的 部 分 1段 细筛 改 造 成 为 2段 细
筛, 在减少细筛总台数 的条件下 , 增加 2段细筛筛分 面积 , 解决 因场地 狭小无法实现增 加细筛 的难题 。 精选 作 业采 用全 自动 淘洗 磁 选 机 , 消 中矿 处 理 系 取
2 1 较差 , 磨 主要 是 因为运 转 中磨机 人 料端 向外溢 矿 , 矿浆重 新返 回细筛 给矿 , 细筛 分级 效 果不 理想 ; 稍 好 , 分 效 率 为 3 .% , 下 产 率 2段 筛 98 筛
为 2% ; 4 3段筛 分效率 仅为 1. 1 , 下产 率 为 04% 筛
由表 6与表 2对 比可 知 , 工 艺 采 用 浓 缩 磁选 原 机脱 水 , 优化 工艺 采 用 水 力 旋 流器 组 达 到 分 级 和 脱 水的效 果 , 2段 磨 机 磨 矿 浓 度 由 6 .8 提 高 到 94 %
7 .2 , 5 4 % 给排 矿 一0 0 4 m 粒 级 含 量 差 值 由 5 .7 m %
76 % ; 筛给 矿 浓 度 高 达 6 % ~6 % , 高 于 正 .9 细 3 5 远 常要 求 的 4 % ; 转 中细 筛 给 矿量 大 , 级 效率 低 , 0 运 分
形成恶性循环 , 使得流程跑 冒现象严重。
段 磨 机能力 发挥 。23段 磨 机磨 矿 效 果 考 查结 果 见 、 表 2 细筛 分级 考查 结果 见表 3 , 。
( 上接第 11页 ) 1
3 结
语
统功能的各项要求 , 大大 的降低 了运行 劳动强度及 维护量 , 足 了选 厂稳 定 运 行 , 高产 量 的要 求 , 满 提 并
MQ 2 7m × . 和 1台 MQ 3 2m X . 溢流 Y . 3 6m Y . 5 4m
铁精矿 7 5万 t , 铁精矿品位为 6 . %。生产 中存在 52 23 、 段细筛分级效率低 , 流程循环负荷大 ,、 2 3段磨 机磨 矿效 率低 、 程 跑 冒严 重 的 问题 。 由于受 厂 房 流 空 间限制 , 法增 加筛 分面 积 , 究采 用水 力旋 流器 无 研 组作为分级设备。2 段磨矿采用水力旋流器组闭路 分级 , 3段磨矿采用水力旋流器组和细筛联合分级 工艺 , 达到了理顺流程 、 稳定铁精矿品位 、 提高系统
产 能 的 目的。
型磨机分别 与 2段高频细筛形成闭路 ; 段 细筛采 1 用 0 1 m筛孔 , 段细筛采用 00 m筛孔 ; .2m 2 .9m 选别 设备采用大筒径磁选机及磁场筛选机 , 原工艺流程
见 图 1 。
原 矿 矿
1 矿石性质
矿石 属 鞍 山式 磁 铁 石 英 岩 , 要 由石 英 、 铁 主 磁 矿 、 闪石 一镁 铁 闪 石 等矿 物 组 成 。矿 石 呈 细 粒 变 铁
13 1
达到 7 % 一 0 6 8 %。优化工艺采用水力旋流器组作
总第 5 8期 1
现 代矿 业
21 0 2年 6月第 6期
格 粒级 含量 , 利 于 提 高 细筛 分 级 效 率 。 同时 利 用 有 细筛 控制最 终 细度 , 克服 了水 力旋 流器 组 的波动 , 稳
定 了精 矿质 量 。
4 优化流 程考查及 应用效果
工 艺 流程 优 化 后 , 运转 效 果 进行 了为 期 1 对 个 月 的考 查化 验 。水 力 旋 流 器组 考查 结 果 见 表 4 细 , 筛 分级 考 查 结 果 见 表 5 3段磨 机 磨 矿 效 果 见 表 6 , , 工 艺优 化前 后生 产 指标对 比结 果见 表 7 。
摘
要
针 对某矿 山存 在 细 筛分级 效率低 , 砂 量 大、 矿 能耗 高等 问题 , 返 磨 通过 采 用水 力 旋 流
器组和 细 筛的联合 分 级 工艺对 选矿 流程进 行优 化 。优化 后 简化 了工 艺流程 , 高 了分级 效 率 , 提 改善
了 2 3段 磨 机磨矿 效 果 , 、 实现 了流程稳 定 顺行 , 到 了提 高磨 机 台效 和铁精 矿 品位 的 目的 。 达 关 键词 水力旋 流 器组 细筛 联 合分 级 工 艺优 化 MQ 2 7m × . G . 3 6m格 子 型磨机 和 1台 MQ 2 7m × G .
由表 5与表 3对 比可 知 , 力旋 流器 组 和细 筛 水 联 合 分 级 工 艺 改 善 了 细 筛 入 筛 物 料 条 件 , 筛 下 在
一
00 4m .7 m含量 保 持 9 %不 变 的条件 下 , 2 筛分 效 率
() 3 利用 水力 旋 流器组 底 流浓度 高 的特 点 , 1段
S ra . 1 e ilNo 5 8
现
代
矿
业
总 第 58 1 期
2 1 年 6月 第 6期 02
J n .2 2 u e 01
M0RD NI EN MI NG
旋 流器 与细筛 联 合 分级 工 艺 在某 铁 矿 的应 用
张润 身 席江 伟 王 磊 , ,
(. 1 河北联合 大学研 究生学院;.河北钢铁集 团矿业有限公 司庙 沟铁矿 ;.威海 市海王旋流 器有限公 司) 2 3
5 结
语
某 磁铁 矿 山通 过采 用 占地 面积 小 、 耗 低 且 更 能 适合 于 细粒分 级 的水力 旋 流器组 和 细筛进 行 联合 分
级, 对选 矿流 程进 行 了优化 , 解决 了原流 程 因恶性 循
m m含量为 7 % , 5 浓度为 4 .6 , 65 % 该物料入筛更有 利 于提 高 细筛 的分级 效率 。
表 1 原 矿 铁 物 相 分 析 结 果 %
2 原工艺流 程及存在 的主要 问题
2 1 原 工 艺流程 .
原 工艺 流程 为 3段 磨 矿 分 级 的 阶段 选 别工 艺 。 磨 机 容 积 按 45: 3配 置 , . 4: 1段 磨 机 采 用 4 台
张润 身 (9 ) 男 , 1一 , 厂长 , 级工程师 ,65 1 高 0 60 河北 省秦皇 岛市
度为 6.l , 5 2 % 2段 水 力 旋 流 器 组 溢 流 中 一0 0 4 .7
由表 7生产 指 标 对 比结 果 可 知 , 流程 优化 后 磨 机平 均 台效提 高 了 2 8 / 台 ・ ) 铁精 矿 品位 提 .2t( , h , 高 了 03个 百分 点 , . 应用 效果 良好 。
表 7. 艺 优 化 前 后 生产 指标 对 比 工
由表 4与 表 3对 比可 知 , 1段水 力 旋 流 器 组 取
代 2段细筛 , 分级效率 由3 .%提高到 6 . 1 , 98 7 1% 分 级粒 度 相 当 , 为提 高磨 机 台效 打下 基 础 ; 水力 旋 2段
流器 组分 级效 率 达到 6 .4 , 49 % 分级 效 果 较好 ; 原流 程 3段 细 筛 人 筛 物 料 一 .7 m 含 量 为 6 % , 0 04m 8 浓