煤质分析报告-中英文
煤质分析报告

53
51
磨损指数Ke
—
1.65
2
本试验报告仅对来样负责
负责人: 审核: 检验:
(专业文档资料素材和资料部分来自网络,供参考。可复制、编制,期待你的好评与关注)
工
业
分
析
空气干燥基水分Mad
%
8.52
8.36
收到基灰分Aar
%
22.61
24.48
收到基挥发分Vdaf
%
49.14
48.66
收到基固定碳Car
%
元
素
分
析
收到基碳Car
%
32.42
31.29
收到基氢Har
%
2.26
2.18
收到基氮Nar
%
0.62
0.6
收到基氧Oar
%
9.76
9.5
收到基全硫Star
%
0.53
0.85
发
热
量
弹筒发热量Qnet.v.ar
J/g
—
—
空干基高位发热量Qnet.v.ar
kJ/kg
—
—
收到基低位发热量Qnet.v.ar
kJ/kg
11710
11290
灰
熔
融
性
变形温度
℃
>1400
2100
软化温度
℃
>1400
2500
半球温度
℃
>1400
------
流动温度
℃
>1400
2900
哈氏可磨性系数HGI
3.65
灰变形温度DT(t1)
℃
ห้องสมุดไป่ตู้>1400
煤炭术语中英文对照

煤炭术语中英文对照煤炭术语中英文对照(一)煤及其产品序号术语名称英文名称定义符号允许使用的同义词停止使用的同义词2.1.1 煤coal 植物遗体在覆盖地层下,压实、转化而成的固体有机可燃沉积岩煤炭2.1.2 煤的品种Categories of coal 以不同方式加工成不同规格的煤炭产品2.1.3 标准煤Coal equivalent 凡能产生29.27MJ 的热量(低位)的任何数量的燃料折合为1kg 标准煤2.1.4 毛煤Run-of-mine coal 煤矿生产出来的,未经任何加工处理的煤2.1.5 原煤Raw coal 从毛煤中选出规定粒度的矸石(包括黄铁矿等杂物)以后的煤2.1.6 商品煤Connercial coal;salable coal 作为商品出售的煤销煤2.1.7 精煤clenedcoal 煤经精选(干选或湿选)后生产出来的、符合质量要求的产品洗精煤2.1.8 中煤Middings 煤经精选后的道德、灰分介于精煤和矸石之间的产品2.1.9 洗选煤Washed coal 经过洗选后的煤'2.1.10 筛选煤Screened coal;sieved coal 经过筛选加工的煤2.1.11 粒级煤Sized coal 煤通过筛选或精选生产的,粒度下限大于6mm 并规定有限下率的产品2.1.12 粒度Size 颗粒的大小2.1.13 限上率Oversize fraction 筛下产品中大于规定粒度上限部分的质量百分数2.1.14 限下率Undersize fraction 筛上产品中小于规定中的粒度下限部分的质量百分数含末率2.1.15 特大块Uitra large coal(>100mm)大于100mm 的粒级煤2.1.16 大块煤Large coal(>50mm)大于50mm 的粒级煤2.1.17 中块煤Medium-sizldcoal(25 ?50mm) 5 ?50mm 的粒级煤2.1.18 小块煤Small coal(13 ?25mm)13 ?25mm 的粒级煤2.1.19 混中块Mixed medium-sized coal (13?80mm)13?80mm 的粒级煤2.1.20 混块Mixedlumpcoal(13 ?300mm) 13 ?300mm 之间的粒级煤2.1.21 粒煤Pea coal(6 ?13mm) 6?13mm 的粒级煤2.1.22 混煤Mixed coal(>0 ?50mm)0?50mm 之间的煤2.1.23 末煤Slack;slackcoal(>0 ?25mm) 0?25mm 之间的煤2.1.24 粉煤Fine coal(>0 ?6mm) 0?6mm 之间的煤2.1.25 煤粉Coal fines(>0 ?0.5mm)小于0.5mm 的煤2.1.26 煤泥slime 煤经洗选或水采后粒度在0.5mm 以下的产品2.1.27 矸石Shale 采.掘过程中从顶、底板或煤层混入煤中的岩石矸子2.1.28 夹矸Dirt band 夹层在煤层中的矿物质层2.1.29 洗矸washeryrejects 从洗煤中排出的矸石2.1.30 含矸率Shale cont ent 煤中大于50mm 矸石的质量百分数(二)煤的采样和制样序号术语名称英文名称定义符号允许使用的同义词停止使用的同义词2.2.1 煤样Coals ample;sample 为确定某些特性而从煤中采取的、具有代表性的一部分煤2.2.2 采样Samping 采取煤样的过程2.2.3 子样Increment 采样器具操作一次或截取一次煤流分断面所采取的一份样2.2.4 总样Gros ssample 从一个采样单元取出的全部子样合并成的煤样2.2.5 随机采样andom sampling 在采取子样式,对采样的部位或时间均不施加任何人为的意志,能使任何部位的煤都有机会采出2.2.6 系统采样Systematic sampling 按相同的时间、空间或质量的间隔采取子样,但第一个子样在第一个间隔内随机采取,其余的子样按选定的间隔采取2.2.7 批Batch;lot 在相同的条件下,在一段时间内生产的一个量2.2.8 采样单元Sampling unit 从一批煤中采取一个总样的煤量。
煤质工业分析报告单

煤质工业分析报告单1. 引言本报告旨在对煤质进行全面的分析和评估,为煤矿和相关工业提供基本的煤炭质量数据。
通过对煤样的化学分析、物理性质测试和燃烧性能评估等方面的考察,可以了解煤炭在工业生产中的潜力和适用性。
2. 煤样来源和采集方法本次煤炭样品采集来源于某煤矿生产过程中的原料煤。
样品采集过程中,我们严格按照标准操作程序进行,保证了样品的代表性和准确性。
在采集过程中,我们遵循以下步骤:1.选择代表性的煤炭样品。
2.通过手工或机械方法进行样品的采集。
3.将采集到的样品放入密封容器中,避免与外界环境接触,以防止质量损失和污染。
3. 化学成分分析3.1 元素含量通过化学分析方法,我们对煤样中的主要元素进行了分析。
以下是元素含量的测试结果:元素含量(%)碳(C)65.2氢(H) 5.8氮(N) 1.2硫(S) 2.6氧(O)25.2灰分(A) 4.53.2 热值分析热值是评价煤炭品质的重要指标之一。
我们使用标准燃烧法,测定了煤样的高位发热量(Q)和低位发热量(Qr)。
测试结果如下:•高位发热量(Q):6500 kcal/kg•低位发热量(Qr):6000 kcal/kg4. 物理性质测试4.1 相对密度煤样的相对密度是描述煤炭重量和体积之间关系的指标。
我们使用比重法测定了煤样的相对密度,结果为1.4 g/cm³。
4.2 粒度分析煤炭的颗粒大小对于燃烧性能和利用价值具有重要影响。
我们使用筛分法对煤样进行了粒度分析,结果如下:•10mm以上:10%•10-5mm:40%•5-1mm:30%•1mm以下:20%5. 燃烧性能评估5.1 燃点分析燃点是指煤炭燃烧的起点温度。
我们使用热重分析法测定了煤样的燃点,结果为350℃。
5.2 燃烧特性煤炭的燃烧特性直接关系到其在工业生产中的应用。
通过对煤样的燃烧试验,我们评估了其燃烧性能,结果如下:•发热速率:10 g/min•燃尽率:90%•灼烧时间:120 min6. 综合评价综合以上测试结果,我们对煤样的工业应用潜力进行了评估。
煤炭术语中英文对照

煤炭术语中英文对照(一)煤及其产品序号术语名称英文名称定义符号允许使用的同义词停止使用的同义词2.1.1煤coal植物遗体在覆盖地层下,压实、转化而成的固体有机可燃沉积岩煤炭2.1.2煤的品种Categories of coal以不同方式加工成不同规格的煤炭产品2.1.3标准煤Coal equivalent凡能产生29.27MJ的热量(低位)的任何数量的燃料折合为1kg标准煤2.1.4毛煤Run-of-mine coal煤矿生产出来的,未经任何加工处理的煤2.1.5原煤Raw coal从毛煤中选出规定粒度的矸石(包括黄铁矿等杂物)以后的煤2.1.6商品煤Connercial coal;salable coal作为商品出售的煤销煤2.1.7精煤clenedcoal煤经精选(干选或湿选)后生产出来的、符合质量要求的产品洗精煤2.1.8中煤Middings煤经精选后的道德、灰分介于精煤和矸石之间的产品2.1.9洗选煤Washed coal经过洗选后的煤'2.1.10筛选煤Screened coal;sieved coal经过筛选加工的煤2.1.11粒级煤Sized coal煤通过筛选或精选生产的,粒度下限大于6mm并规定有限下率的产品2.1.12粒度Size颗粒的大小2.1.13限上率Oversize fraction筛下产品中大于规定粒度上限部分的质量百分数2.1.14限下率Undersize fraction筛上产品中小于规定中的粒度下限部分的质量百分数含末率2.1.15特大块Uitra large coal(>100mm)大于100mm的粒级煤2.1.16大块煤Large coal(>50mm)大于50mm的粒级煤2.1.17中块煤Medium-sizldcoal(25~50mm)5~50mm的粒级煤2.1.18小块煤Small coal(13~25mm)13~25mm的粒级煤2.1.19混中块Mixed medium-sized coal(13~80mm)13~80mm的粒级煤2.1.20混块Mixedlumpcoal(13~300mm)13~300mm之间的粒级煤2.1.21粒煤Pea coal(6~13mm)6~13mm的粒级煤2.1.22混煤Mixed coal(>0~50mm)0~50mm之间的煤2.1.23末煤Slack;slackcoal(>0~25mm)0~25mm之间的煤2.1.24粉煤Fine coal(>0~6mm)0~6mm之间的煤2.1.25煤粉Coal fines(>0~0.5mm)小于0.5mm的煤2.1.26煤泥slime煤经洗选或水采后粒度在0.5mm以下的产品2.1.27矸石Shale采.掘过程中从顶、底板或煤层混入煤中的岩石矸子2.1.28夹矸Dirt band夹层在煤层中的矿物质层2.1.29洗矸washeryrejects从洗煤中排出的矸石2.1.30含矸率Shale cont ent煤中大于50mm矸石的质量百分数(二)煤的采样和制样序号术语名称英文名称定义符号允许使用的同义词停止使用的同义词2.2.1煤样Coals ample;sample为确定某些特性而从煤中采取的、具有代表性的一部分煤2.2.2采样Samping采取煤样的过程2.2.3子样Increment采样器具操作一次或截取一次煤流分断面所采取的一份样2.2.4总样Gros ssample从一个采样单元取出的全部子样合并成的煤样2.2.5随机采样andom sampling在采取子样式,对采样的部位或时间均不施加任何人为的意志,能使任何部位的煤都有机会采出2.2.6系统采样Systematic sampling按相同的时间、空间或质量的间隔采取子样,但第一个子样在第一个间隔内随机采取,其余的子样按选定的间隔采取2.2.7批Batch;lot在相同的条件下,在一段时间内生产的一个量2.2.8采样单元Sampling unit从一批煤中采取一个总样的煤量。
主要煤质指标分级标准与煤质分析报告

煤质分析部分一部分:煤质概况(一)煤及其产品(七)煤质分析常用数理统计术语 ?????????(八)煤炭粒度分级煤和褐煤的分级 1.长焰煤,不粘煤、弱粘煤、气煤、瘦煤、贫煤和无烟煤,根据粒度不同分为下列各级:注:1)本标准不规定焦煤、肥煤以及全部作为炼焦配煤用的气煤和瘦煤的粒度级别,但焦煤肥煤作燃料直接使用而用户又要求分级时,其粒度尺寸应符合本标准的规定。
2)当长烟煤、不粘煤、弱粘煤、气煤、瘦煤、贫煤和无烟煤的水分较高或者用于粉煤燃烧装置,不能或不需要筛出6~13毫米的煤炭时,可生产小于13毫米的煤炭,称为抹煤,符号为M。
3)各级煤炭的限下含量,应符合煤炭产品质量标准的规定。
2.褐煤根据粒度不同,分为下列各级:(八)煤炭粒度分级煤和褐煤的分级 1.长焰煤,不粘煤、弱粘煤、气煤、瘦煤、贫煤和无烟煤,根据粒度不同分为下列各级:注:1)本标准不规定焦煤、肥煤以及全部作为炼焦配煤用的气煤和瘦煤的粒度级别,但焦煤肥煤作燃料直接使用而用户又要求分级时,其粒度尺寸应符合本标准的规定。
2)当长烟煤、不粘煤、弱粘煤、气煤、瘦煤、贫煤和无烟煤的水分较高或者用于粉煤燃烧装置,不能或不需要筛出6~13毫米的煤炭时,可生产小于13毫米的煤炭,称为抹煤,符号为M。
3)各级煤炭的限下含量,应符合煤炭产品质量标准的规定。
2.褐煤根据粒度不同,分为下列各级:*在已确定无烟煤小类的生产矿、厂的日常工作中,可以只按Vr分类;在地址勘探工作中,为新区确定小类或生产矿、厂和其他单位需要重新核定小类时,应同时测定Vr和Hr,按上表小类。
如两种结果有矛盾,以按Hr划小类的结果为准。
表4 烟煤的分类*当烟煤的粘结指数测值G小于或等于85时,用于干燥无灰基挥发分V和粘结指数G来划分煤类。
当粘结支书测值G大于85时,则用干燥无灰基挥发分V和胶质层最大厚度Y,或用干燥无灰基挥发分V和奥亚膨胀度b来划分煤类。
**当G>85时,用Y和b并列作为分类指标。
煤全分析报告

煤全分析报告报告概述:本煤全分析报告是根据客户所提供的样品进行的分析测试。
通过测试,我们对该煤种样品的物理、化学属性、热值等参数进行了详细的分析,从而为客户提供准确可靠的数据和评估。
样品情况:该样品为煤炭常用的一种掘进工业利用煤,样品重量为50克。
在分析测试之前,我们先对该样品进行了粉碎、筛分和干燥处理,以确保测试结果的准确性。
分析测试结果:1.物理属性物理属性是反映样品物理状态的一些基本特征,主要包括颗粒大小、比重和磨损等指标。
在测试中,我们使用标准方法对该样品的物理属性进行了测定。
测试结果表明:该煤种样品颗粒主要以0.1-0.25mm为主,75%的颗粒径在0.1-0.5mm之间。
该煤种样品的绝对密度为1.35g/cm³,相对密度为1.65g/cm³。
在磨损实验中,该煤种样品平均磨损率为3.4g/kg,属于较低的磨损性质。
2.化学属性化学属性是煤种样品中主要元素和化学组成的反映,主要包括含氢量、含氧量、含硫量等指标。
在测试中,我们使用标准方法对该样品的化学属性进行了测定。
测试结果表明:该煤种样品的含氢量为5.3%,含氧量为12.6%,含硫量为1.2%。
该煤种样品的灰分含量为15.2%,属于较高的灰分含量。
3.热值热值是煤种样品燃烧所释放的热量能,也称为热功值。
在测试中,我们使用标准方法对该样品的热值进行了测定。
测试结果表明:该煤种样品的热值为5200 kcal/kg,属于一般的热值水平。
结论:综上所述,该煤种样品在物理、化学属性方面表现出较好的特性,但灰分含量较高,对锅炉设备有一定的腐蚀和磨损作用。
热值水平方面属于一般水平,适合于一般锅炉和热处理设备使用。
针对该煤种样品的特性,我们建议客户在实际使用过程中,进行适当的调整和处理,以提升其综合利用价值。
报告编号:20210928报告日期:2021年9月28日测试单位:XXXXXX分析中心测试人员:XXX、XXX、XXX。
煤质分析报告

DT(t1)
c
>1400
2100
灰软化温度
ST(t2)
c
>1400
2500
灰熔化温度
FT(t3)
c
>1400
2900
煤质分析试验报告
送样单位
内蒙古兴安银铅冶炼有限公司
样品名称
白音华2号露天煤矿原煤
送样时间
报告日期
报告编号
项目名称
单位
试验结果
设计煤种
校核煤种
全水分Mt
%
31.8
31.1
工 业 分 析
48.66
空气干燥基水份
Mad
%
8.52
8.36
兀素分析
收到基碳
Car
%
32.42
31.29
收到基氢
Har
%
2.26
2.18
收到基氧
Oar
%
9.76
9.5
收到基氮
Nar
%
0.62
0.6
收到基硫
Star
%
0.53
0.85
哈氏可磨性系数
HGI
一
53
51
磨损指数
Ke
一
1.65
2
游离二氧化硅
2.45
3.65
本工程燃煤来源为白音华2号露天煤矿,煤质成分分析见表4.1-1。
表4.1-1
煤质成分分析
煤源:白音华
项目
单位
设计煤种
校核煤种
收到基低位发热值
Qn et.v.ar
kJ/kg
11710
11290
工业分析
收到基全水份
Coal Analysis Data(煤分析的数据)

1.8 Coal Physical Properties and Petrographic FeaturesFrom the viewpoints of petrography, coal is a hydrocarbon. Consequently, the methods for study petrography can be applied to the qualitative and quantitative analysis to the coal physical properties and petrographic composition for guiding the processing and utilization.1.8.1 Coal Physical PropertiesEach coal seam of No. 7, 6, 5 (5upper), 4 (4 upper) and 1 is characterized by brown and black-brown color, and sometimes light brow, dark brown and black color. The streaks is mainly in light brown and yellowish brown color, sometimes in dark brown color with weak-strong asphalt luster and weak greasy luster. The coal is mainly massive, and the breaking-faces are always in shell and irregular shapes. The maceral of the coal seams consists of mainly dull coal and secondly bright coal with a little vitrain and fusinite. The external fissures are well developed in most directions in paralleled or approximately paralleled to the core axes. The other physical properties are shown in Table 3-1-1.Table of the physical properties of the mineable coal seams1.8.2 Coal Petrographic Features1.8.2.1 Macroscopic Coal Petrographic FeaturesThe macroscopic coal petrographic features is identified by naked eye or by magnifying glass on the appearance characteristics, such as coal color, streaks color, luster, streaks, hardness and etc. The coal petrographic components mainly include vitrain, clarain, durain and fusinite. Vitrain and fusinite are the simple components of coal, and the clarain anddurain are the complicated components of coal. Based on the proportions, combined conditions and the average intensity of luster, the maceral types can be divide into four type as bright, semi-bright, semi-dull and dull.The coal seams of 7, 6, 5 (5upper), 4 (4 upper) and 1 mainly consist of semi-dull and dull type coal, few semi-light type coal. Durain is its main maceral component, which always exists in coal seams in thick state. Clarain is its secondary component, vitrain and fusinite only covers a very few amount. The secondary component always exits in coal seams in thin lamellar and lineation state.1.8.2.2 Microscopic Coal Petrographic FeaturesThe microscopic coal petrographic features are obtained by microscope. Coal are cut into thin slice and observed on the color, texture, shape, transparency and outline etc. under transmission light or cut into polished slice to be observed on the color, structure, shape, tuber and reflectance under the reflected light. The sequence of study on maceral components is generally from macro to micro. The petrographic features are measured on the separated component respectively. The maceral components consist of organic component converted from plant and inorganic component converted from minerals.(1) Organic ComponentThe organic components of coal seams No. 7, 6, 5 (5upper), 4 (4 upper) and 1 are mainly huminite, secondly inertinite and liptinite, which are shown in Table 3-1-2. The table indicates the huminite and inertinite contents of coal seam No. 6 are the highest, the huminite and inertinite contents of coal seam No. 7 is lower than other coal seams. The liptinite content of coal seam No. 7 and 5 (5upper) is relatively high, and the content of coal seam No. 7 and 4 (4 upper) is the lowest. The detailed are described as follows:①Huminite: It is the mianly component of the maceral components, its content of each coal seam is greater than 57%, the highest even reaches 87.59%, which mainly consists of homocollinite, secondly humotelinite and humodetrinite.②Humocollinite mainly consists of gelinite in state of cements and telogelinite,secondly corpohuminite.③Humotelinite mainly consists of woody structure ulminite and fully decomposed ulminite, and little textinite (cell empty or filled with clay, micro-sized particles, lipoid and little gelinite).Each coal seam contains mainly sclerotinite (monoatrial and polytrial) and rare fusinite fragments.Each coal seam contains mainly tenuicutinite, suberinite, bituminite (granular matrix in vein texture), and secondly sporinite and resinite.(2) Inorganic ComponentsThe inorganic components include clay, sulfide, oxide and carbonate. The clay is the majority, which is often distributed in impregnated and banded structures and minor flake shape. The sulfide is mainly pyrite distributed in fine particle, crystal grain and sphaerolitic shape or aggregation, minor in filling, lump, framboidal shapes. Binarite is minor. The quartz are the main component in oxide in granular and angular shape. Diatom is not often seen, but quartz and diatom fossil are combined together are often seen. The carbonate, only coal seam 1 meets calcite in flake. The organic components contents are shown in Table 3-1-2.A table of microscopic petrographic contentTable 3-1-2Coal seam (Point number)Test items7 (2) 6 (6) 5 (5upper) (5) 4 (4upper) (4) 1 (5)Huminite 64.18-68.8066.4975.01-87.5979.4570.44-79.3275.4157.82-85.5375.0160.01-81.2771.38Humocollinite 0.50-0.990.751.44-3.372.260.85-3.251.731.00-2.581.680.59-2.561.98Humotelinite 14.60-17.3315.975.89-17.1912.539.24-23.0115.584.17-12.169.3211.06-19.4813.88clay 7.7-12.810.25 0.1-5.01.831.0-9.03.420.0-27.79.630.7-18.79.14oxide 2.3-6.44.35 1.2-4.12.420.3-2.51.181.1-3.21.980.4-2.31.20carbonate 0.0 0.0-0.40.16 0.0 0.00.0-2.40.94sulfide 1.0-3.42.20 0.4-4.61.361.9-3.12.680.6-4.42.400.3-5.01.481.8.2.3 Microscopic Petrographic Structure and typeEach coal seam is characterized by banded structure observed under the microscope. According to the different combination of the maceral concentrates determined by the microscopic observation, the humic coal can be divided into vitrite, fusitoid, clarotelite, durite and other various transitional types. The microscopic petrographic type of the coal in the project area is mainly vitrite, secondly clarotelite. The microscopic mineralization type is mainly micro clay coal, micro sulphuration coal. The microscopic minerals type of micro clay and micro sulphuration can be found.1.8.2.4 Maximum Reflectance of Huminite and metamorphic stageThe maximum reflectance of huminite (R0 max) ranges from 0.29% to 0.36%, indicating the metamorphic grade of coal seams in the project area is low, the deep seated metamorphism of coal seams is not noticeable, the coal seams is in 0 metamorphic stage(Table 3-1-3).Result table of 3.1.2.4 Maximum Reflectance of HuminiteTable3-1-3The main coal quality test specifications of the main mineable coal seams are shown in Table 3-2-1, and the changes on vertical direction are shown in Fig. 3-2-1.Fig.3-2-1 Diagram of the vertical changes of coal quality indexes of the each mineable coal seam1.9.1 Moisture Content (M ad )The moisture in coal can be divided into two types of inherent moisture and extraneous moisture based on the different states of the moisture. The inherent moisture is totally evaporated above the temperature of 100℃, the external moisture is evaporated at the temperature of 45-50℃. The coal is completely evaluated on air dried basis, which the extraneous moisture is lost. The average moisture content of the raw coal is about 16.56-19.40% ranging from 8.15% to 24.66%. The average moisture content of the floated coal is about 11% ranging from 7.82% to 19.25%, indicating a little bit lower than that of the raw coal. The moisture content of the lignite is generally lower than the moisture content of the raw coal. For the low-rank coal, because the moisture content of the organic mater greater than the moisture content in the minerals, so when the content of the minerals is higher, the inherent moisture content will be lower, which is a inverse relation. The moisture content is harmful to the industrial utilization of coal. During the coal storage, the air moisture content will influence the moisture content in coal, which will make the coal easily broken and accelerate the coal oxidation.Coal seam 7 6 5 (5upper ) 4 (4upper ) 1 R 0,max (%)0.31-0.35 0.33 (2)0.30-0.33 0.31 (6)0.29-0.35 0.32 (5)0.30-0.35 0.32 (4)0.29-0.36 0.33 (5)本页已使用福昕阅读器进行编辑。